JAW INSPECTION AND MAINTENANCE
JAW AND TOOTH REBUILD PROCEDURE: S, C, and G JAWS
Welding Rod: Airco Tubecraft 1A, Cronatron 7355, Eutectic N6006, Postalloy 214,
Stoody 31 or equal. In Canada: NCH Canada Inc. Wear-X #176 or equal.
Dry welding rod at 300°F+
(150°C+)
.
Pre-heat the jaw weld area to 350°F
(177°C)
and maintain this temperature
during the welding operation. It is very important to maintain this temperature in
cold environments.
Adjust weld current to rod manufacturer’s specifications.
Peen each layer. Do not exceed 2 – 3 layers of hard face.
Cool slowly. Cover weld in cold environments.
DO NOT WELD OVER OLD HARDFACING!
Remove all old hard facing before applying new underlay weld.
1. BEFORE WELD
2. AFTER WELD
CORRECT
BD/BI
MALE OR FEMALE
CRUSHER JAW
DI
WORN AREA
we2
UNDERLAYMENT
we3
HARDFACE
CORRECT
BD/BI
MALE OR FEMALE
CRUSHER JAW
we2
UNDERLAYMENT
we3
HARDFACE
we5
END OF NEW
WELD
we6
OLD WELD
73
FINISH GRIND TO
BLEND
INCORRECT
BD/BI
MALE OR FEMALE
CRUSHER JAW
we4
OVERFLOW
we5
END OF NEW
WELD
Содержание M20C
Страница 23: ... 23 SERIAL NUMBER LOCATION M20 ...
Страница 24: ... 24 SERIAL NUMBER LOCATION M28 ...
Страница 25: ... 25 SERIAL NUMBER LOCATION M38 ...
Страница 149: ... 149 WARRANTY STATEMENTS ...
Страница 150: ... 150 WARRANTY STATEMENTS ...
Страница 152: ... Copyright 2018 NPK Construction Equipment Inc www npkce com M000 9600I 10 18 Material Processor Instruction Manual ...