JAW INSPECTION AND MAINTENANCE
JAW AND TOOTH REBUILD PROCEDURE: S, C, and G JAWS
2. UNDERLAYMENT
Underlayment weld is necessary to build-up the base material (DH) to match the
original jaw or tooth profile before hard facing. You cannot hard face over old hard
facing.
Welding rod: Airco Austex 361, Cronatron 7770, Eutectic 3205, Postalloy 205,
Stoody 2110 or equal. In Canada: NCH Canada Inc. Hi-Pact #194 or equal.
Dry welding rod at 300°F+
(150°C+)
.
Pre-heat the jaw area to 300° - 400°F
(150° - 200°C)
and maintain this
temperature during the welding operation. It is very important to maintain this
temperature in cold environments.
Adjust weld current to rod manufacturer’s specifications.
Peen each layer.
Cool slowly. Cover weld in cold environments.
3. HARDFACE
Hardface (we3) can only be applied over base material (DH) or underlayment weld
(we2).
NEVER HARDFACE OVER EXISTING HARDFACE!
Содержание M20C
Страница 23: ... 23 SERIAL NUMBER LOCATION M20 ...
Страница 24: ... 24 SERIAL NUMBER LOCATION M28 ...
Страница 25: ... 25 SERIAL NUMBER LOCATION M38 ...
Страница 149: ... 149 WARRANTY STATEMENTS ...
Страница 150: ... 150 WARRANTY STATEMENTS ...
Страница 152: ... Copyright 2018 NPK Construction Equipment Inc www npkce com M000 9600I 10 18 Material Processor Instruction Manual ...