64
-
JAW INSPECTION AND MAINTENANCE
JAW INSPECTION: G and S JAWS
WEEKLY INSPECTION
JAW AND TOOTH REBUILD PROCEDURE: S and G JAWS
Welding Rod: Airco Tubecraft 1A, Cronatron 7355, Eutectic N6006, Postalloy 214,
Stoody 31 or equal. In Canada: NCH Canada Inc. Wear-X #176 or equal.
Dry welding rod at 300°F+
(150°C+)
.
Pre-heat the jaw area to 350°F
(177°C)
and maintain this temperature during the
welding operation. It is very important to maintain this temperature in cold
environments.
Adjust weld current to rod manufacturer’s specifications.
Peen each layer. Do not exceed 2 – 3 layers of hard face.
Cool slowly. Cover weld in cold environments.
DO NOT WELD OVER OLD HARDFACING!
Remove all old hardfacing before applying new underlay weld.
1. BEFORE WELD
2. AFTER WELD
CORRECT
BD/BI
MALE OR FEMALE
CRUSHER JAW
DI
WORN AREA
we2
UNDERLAYMENT
we3
HARD FACE
CORRECT
BD/BI
MALE OR FEMALE
CRUSHER JAW
we2
UNDERLAYMENT
we3
HARD FACE
we5
END OF NEW WELD
we6
OLD WELD
73
FINISH GRIND TO
BLEND
INCORRECT
BD/BI
MALE OR FEMALE
CRUSHER JAW
we4
OVERFLOW
we5
END OF NEW
WELD