Porosity of weld seam
Spattering in the gas nozzle, causing inadequate gas shield for weld seam
Remove welding spatter
Holes in gas hose or imprecise gas hose connection
Replace gas hose
O-ring at central connector is cut or faulty
Replace O-ring
Moisture/condensate in the gas line
Dry gas line
Gas flow too strong or weak
Correct gas flow
Inadequate quantity of gas at the start or end of welding
Increase gas pre-flow and gas post-flow
Too much parting agent applied
Remove excess parting agent/apply less parting agent
Cause:
Remedy:
Cause:
Remedy:
Cause:
Remedy:
Cause:
Remedy:
Cause:
Remedy:
Cause:
Remedy:
Cause:
Remedy:
Poor ignition properties
Unsuitable tungsten electrode (e.g., WP electrode for DC welding)
Use suitable tungsten electrode
Wearing parts loose
Screw on wearing parts tightly
Cause:
Remedy:
Cause:
Remedy:
Gas nozzle is cracked
Tungsten electrode not protruding far enough out of the gas nozzle
Have tungsten electrode protrude more out of the gas nozzle
Cause:
Remedy:
94
Summary of Contents for HPT 220i G
Page 2: ......
Page 10: ...User Interface tauschen User Interface austauschen 1 3 2 1 2 1 3 2 0 6Nm 3 10...
Page 15: ...Spanneinheit montieren 3 30 1 4 2 1 PUSH Wolframelektrode montieren 5 1 2 6 15 DE...
Page 16: ...2 2 d d 1 7 16...
Page 19: ...2 1 3 5 6 7 4 1 nur bei wassergek hltem Schwei system 19 DE...
Page 40: ...Pflege Wartung und Entsorgung Verbote 40...
Page 52: ...52...
Page 60: ...Replacing the user interface Replacing the user interface 1 3 2 1 2 1 3 2 0 6Nm 3 60...
Page 65: ...Fit the clamping unit 3 30 1 4 2 1 PUSH Fit the tungsten electrode 5 1 2 6 65 EN US...
Page 66: ...2 2 d d 1 7 66...
Page 69: ...2 1 3 5 6 7 4 1 only with water cooled welding system 69 EN US...
Page 90: ...Service maintenance and disposal Prohibited 90...
Page 102: ...102...
Page 116: ...2 2 d d 1 7 116...
Page 119: ...2 1 3 5 6 7 4 1 nicamente con sistema de soldadura enfriado con agua 119 ES MX...
Page 140: ...Cuidado mantenimiento y desecho Prohibido 140...
Page 152: ...152...
Page 165: ...Monter l unit de serrage 3 30 1 4 2 1 PUSH Monter l lectrode en tungst ne 5 1 2 6 165 FR...
Page 166: ...2 2 d d 1 7 166...
Page 169: ...2 1 3 5 6 7 4 1 uniquement pour le syst me de soudage refroidi par eau 169 FR...
Page 191: ...Maintenance entretien et limination Interdictions 191 FR...
Page 210: ...Bytte grensesnitt Bytte grensesnitt 1 3 2 1 2 1 3 2 0 6Nm 3 210...
Page 215: ...Montere spennenheten 3 30 1 4 2 1 PUSH Montere wolframelektroden 5 1 2 6 215 NO...
Page 216: ...2 2 d d 1 7 216...
Page 219: ...2 1 3 5 6 7 4 1 kun p vannkj lte sveisesystemer 219 NO...
Page 236: ...Sperre bytte av pistolkroppen Sperre bytte av sveispistolenhet 1 3 2 1 1 2 2 1 3 0 6Nm 2 3 236...
Page 240: ...Pleie vedlikehold og avhending Forbud 240...
Page 252: ...252...
Page 265: ...Montar a unidade de tens o 3 30 1 4 2 1 PUSH Montar o eletrodo de tungst nio 5 1 2 6 265 PT BR...
Page 266: ...2 2 d d 1 7 266...
Page 269: ...2 1 3 5 6 7 4 1 Somente com o sistema de soldagem refrigerado a gua 269 PT BR...
Page 290: ...Conserva o Manuten o e Descarte Proibido 290...
Page 302: ...302...
Page 303: ...303 PT BR...