TRANSTIG 300 AC/DC
SERVICE MANUAL
10-6
June 30, 2008
Description Possible
Cause
Remedy
5 Non-metallic
particles
are trapped in the
weld metal (slag
inclusion).
A Non-metallic particles may be
trapped in undercut from
previous run.
A If bad undercut is present, clean
slag out and cover with a run
from a smaller diameter electrode.
B Joint preparation too restricted.
B Allow for adequate penetration
and room for cleaning out
the slag.
C Irregular deposits allow slag to
be trapped.
C If very bad, chip or grind out
irregularities.
D Lack of penetration with slag
trapped beneath weld bead.
D Use smaller electrode with
sufficient current to give adequate
penetration. Use suitable tools to
remove all slag from corners.
E Rust or mill scale is preventing
full fusion.
E Clean joint before welding.
F Wrong electrode for position in
which welding is done.
F Use electrodes designed for
position in which welding is done,
otherwise proper control of slag
is difficult.
Table 10-2 (continued): Stick Welding Problems
Not cleaned, or
incorrect
electrode
Slag trapped in
undercut
Art # A-04993
Slag trapped in root
Figure 10-3: Examples of Slag Inclusion
Summary of Contents for TRANSTIG 300 AC/DC
Page 8: ......
Page 20: ...TRANSTIG 300 AC DC SERVICE MANUAL 2 6 June 30 2008 THIS PAGE LEFT INTENTIONALLY BLANK...
Page 34: ...TRANSTIG 300 AC DC SERVICE MANUAL 5 2 June 30 2008 NOTES...
Page 56: ...TRANSTIG 300 AC DC SERVICE MANUAL 11 2 June 30 2008 NOTES...
Page 78: ...THIS PAGE LEFT INTENTIONALLY BLANK TRANSTIG 300 AC DC SERVICE MANUAL 13 18 June 30 2008...
Page 125: ...THIS PAGE LEFT INTENTIONALLY BLANK TRANSTIG 300 AC DC SERVICE MANUAL June 30 2008 A 7...