ENGLISH
OM-363 Page 59
SECTION 9
−
SELECTING AND PREPARING A TUNGSTEN
FOR DC OR AC WELDING
gtaw_Phase_2007
−
04
!
Whenever possible and practical, use DC weld output instead of AC weld output.
9-1. Selecting Tungsten Electrode (
Wear Clean gloves To Prevent Contamination Of Tungsten
)
Amperage Range - Gas Type
♦
- Polarity
Electrode Diameter
(DCEN)
−
Argon
Direct Current Electrode Negative
(For Use With Mild Or Stainless Steel)
AC
−
Argon
Balance Control @ 65% Electrode Negative
(For Use With Aluminum)
2% Ceria (Orange Band), 1.5% Lanthanum (Gray Band), Or 2% Thorium (Red Band) Alloy Tungstens
.040” (1 mm)
25-85
20-80
1/16” (1.6 mm)
50-160
50-150
3/32” (2.4 mm)
135-235
130-250
1/8” (3.2 mm)
250-400
225-360
Pure Tungsten (Green Band)
.040” (1 mm)
Pure Tungsten Not Recommended
For DCEN
−
Argon
10-60
1/16” (1.6 mm)
50-100
3/32” (2.4 mm)
100-160
1/8” (3.2 mm)
150-210
♦
Typical argon shielding gas flow rates are 11 to 35 cfh (cubic feet per hour).
Figures listed are a guide and are a composite of recommendations from American Welding Society (AWS) and electrode manufacturers.
9-2. Preparing Tungsten Electrode For Welding With Phase Control Machines
!
Grinding the tungsten electrode produces dust and flying sparks which can cause injury and start fires. Use
local exhaust (forced ventilation) at the grinder or wear an approved respirator. Read MSDS for safety infor-
mation. Consider using tungsten containing ceria, lanthana, or yttria instead of thoria. Grinding dust from
thoriated electrodes contains low-level radioactive material. Properly dispose of grinder dust in an environ-
mentally safe way. Wear proper face, hand, and body protection. Keep flammables away.
A. Preparing Tungsten For DC Electrode Negative (DCEN) Welding
Ideal Tungsten Preparation
−
Stable Arc
2-1/2 Times
Electrode Diameter
1
Grinding Wheel
Grind end of tungsten on fine grit, hard
abrasive wheel before welding. Do not use
wheel for other jobs or tungsten can become
contaminated causing lower weld quality.
2
Tungsten Electrode
A 2% ceriated tungsten is recommended.
3
Flat
Diameter of this flat determines amperage
capacity.
4
Straight Ground
Grind lengthwise,
not radial
.
1
3
4
1
Tungsten Electrode
A pure tungsten is recommended..
2
Balled End
Ball end of tungsten by applying AC amper-
age recommended for a given electrode
diameter (see Section 9-1). Let ball on end of
the tungsten take its own shape.
B. Preparing Tungsten For AC Welding
1
−
1-1/2 Times
2
Electrode Diameter
Causes Wandering Arc
2
1
Wrong Tungsten Preparation
Radial Grinding
Summary of Contents for Syncrowave 250 DX
Page 6: ......
Page 35: ...ENGLISH OM 363 Page 29 Notes...
Page 43: ...ENGLISH OM 363 Page 37 CE Nameplate E 2 1 2 3 4...
Page 47: ...ENGLISH OM 363 Page 41 CE Nameplate 00 4 SEL 1 4 2...
Page 61: ...ENGLISH OM 363 Page 55 231 395 B Figure 7 2 Circuit Diagram For 350 LX Models...
Page 62: ...OM 363 Page 56 225 650 A Figure 7 3 Circuit Diagram For Optional Cooler...
Page 69: ...ENGLISH OM 363 Page 63 Notes...
Page 80: ...Notes...