Sample Programs
Name
Ramp 1
t1
Soak time
Ramp 2
Soak temp
Low Biscuit
70°C/hr
600°C
00:15
FULL
960°C
Normal Biscuit
70°C/hr
600°C
00:15
FULL
1000°C
High Biscuit
70°C/hr
600°C
00:15
FULL
1160°C
Earthenware Low
Temperature Glaze
90°C/hr
600°C
00:30
FULL
960°C
Earthenware Mid
Temperature Glaze
90°C/hr
600°C
00:30
FULL
1040°C
Earthenware High
Temperature Glaze
90°C/hr
600°C
00:30
FULL
1140°C
Stoneware Glaze
90°C/hr
600°C
00:30
FULL
1250°C
On Glaze Enamel
90°C/hr
600°C
00:30
FULL
780°C
Heavy Sculpture
50°C/hr
300°C
00:30
70°C/hr
1000°C
Lustre
90°C/hr
600°C
00:00
FULL
750°C
Sample
Pr
ogram
s
Notes
Earthenware High Temperature Glaze is also suitable for Stoneware Low
Temperature Glaze.
Stoneware Glaze is also suitable for Porcelain.
On Glaze Enamel is also suitable for some enamelling work.
Heavy Sculpture is also suitable for Terracotta.