33/69
Gala Gar, S.L. c/ Jaime Ferrán, 19 (Políg. Cogullada) | Tel.: (+34) 976 47 34 10 - 50014 ZARAGOZA |
SMART MIG 350 MPV1
9.3. Parameters for fillet welding in the vertical position
Plate
thickness
t (mm)
Bead size
I (mm)
Wire
diameter
(mm)
Welding
current
(A)
Welding
voltage
(V)
Welding
speed
(cm/min)
Gas flow
(l/min)
1.2
2.5~3.0
1.0
70~100
18~19
50~60
10~15
1.6
2.5~3.0
1.0 ~ 1.2
90~120
18~20
50~60
10~15
2.0
3.0~3.5
1.0 ~ 1.2
100~130
19~20
50~60
10~20
2.3
3.0~3.5
1.0 ~ 1.2
120~140
19~21
50~60
10~20
3.2
3.0~4.0
1.0 ~ 1.2
130~170
22~22
45~55
10~20
4.5
4.0~4.5
1.2
200~250
23~26
45~55
10~20
9.4. Parameters for Lap Welding
Plate
thickness
t (mm)
Welding
position
Wire
diameter
(mm)
Welding
current
(A)
Welding
voltage
(V)
Welding
speed
(cm/min)
Gas flow
(l/min)
1.2
A
1.0
80~100
18~19
45~55
10~15
1.6
A
1.0 ~ 1.2
100~120
18~20
45~55
10~15
2.0
A or B
1.0 ~ 1.2
100~130
18~20
45~55
15~20
2.3
B
1.0 ~ 1.2
120~140
19~21
45~50
15~20
3.2
B
1.0 ~ 1.2
130~160
19~22
45~50
15~20
4.5
B
1.2
150~200
21~24
40~45
15~20