Annealing
Annealing is a very important post-processing procedure for PA12 CF.
Through annealing, FFF process induced inner-stress of PA12 CF can be
released.
Annealing accelerates the post-crystallization process and improve stiffness and
dimensional stability for end-use.
Place the printed part together with support material into a dying oven.
Set the oven temperature at 80 ℃ for the annealing.
Avoid any direct contact on hot surface in the oven chamber (may lead to materi-
al melting).
Normally, the annealing time depends on the size of printed part, at least for
6-8h.