![Thermal Arc pro-life 250s Operating Manual Download Page 46](http://html1.mh-extra.com/html/thermal-arc/pro-life-250s/pro-life-250s_operating-manual_1103195046.webp)
4 Portions of the
weld run do not
fuse to the surface
of the metal or
edge of the joint.
A
B
Small electrodes used on
heavy cold plate.
Welding current is too low.
A
B
Use larger electrodes and pre-
heat the plate.
Increase welding current
C Wrong electrode angle.
C Adjust angle so the welding
arc is directed more into the
base metal
D
Travel speed of electrode is
too high.
D Reduce travel speed of
electrode
E Scale or dirt on joint surface. E Clean surface before welding.
Figure 9 – Example of lack of fusion
5 Non-metallic parti-
cles are trapped in
the weld metal
(slag inclusion).
A Non-metallic particles may
be trapped in undercut from
previous run.
A If bad undercut is present,
clean slag out and cover with a
run from a smaller diameter
electrode.
B
Joint preparation too
restricted.
B Allow for adequate
penetration and room for
cleaning out the slag.
C
Irregular deposits allow slag
to be trapped.
C If very bad, chip or grind out
irregularities.
D
Lack of penetration with slag
trapped beneath weld bead.
D Use smaller electrode with
sufficient current to give
adequate penetration. Use
suitable tools to remove all
slag from corners.
E
Rust or mill scale is
preventing full fusion.
E Clean joint before welding.
F
Wrong electrode for position
in which welding is done.
F Use electrodes designed for
position in which welding is
done, otherwise proper control
of slag is difficult.
Figure 10 – Examples of slag inclusion
PRO-LITE 250S
June 29, 2005
46
Summary of Contents for pro-life 250s
Page 2: ......
Page 16: ...THIS PAGE LEFT INTENTIONALLY BLANK ...
Page 28: ...PAGE LEFT INTENTIONALLY BLANK PRO LITE 250S June 29 2005 28 ...
Page 56: ...APPENDIX A INTERCONNECT DIAGRAM PRO LITE 250S June 29 2005 56 ...
Page 57: ...PRO LITE 250S 57 June 29 2005 ...
Page 59: ...Figure 11 Location of PCB WK 4921 PRO LITE 250S 59 June 29 2005 ...
Page 60: ......