OM-227 978 Page 37
9-14. Troubleshooting
−
Waviness Of Bead
Waviness Of Bead
−
weld metal that is not parallel and does not cover
joint formed by base metal.
S-0641
Possible Causes
Corrective Actions
Welding wire extends too far out of nozzle.
Be sure welding wire extends not more than 1/2 in (13 mm) beyond nozzle.
Unsteady hand.
Support hand on solid surface or use two hands.
9-15. Troubleshooting
−
Distortion
Distortion
−
contraction of weld metal during welding that forces
base metal to move.
Base metal moves
in the direction of
the weld bead.
S-0642
Possible Causes
Corrective Actions
Excessive heat input.
Use restraint (clamp) to hold base metal in position.
Make tack welds along joint before starting welding operation.
Select lower voltage range and/or reduce wire feed speed.
Increase travel speed.
Weld in small segments and allow cooling between welds.
9-16. Common MIG Shielding Gases
This is a general chart for common gases and where they are used. Many different combinations (mixtures) of
shielding gases have been developed over the years. The most commonly used shielding gases are listed in the
following table.
Application
Gas
Spray Arc Steel
Short Circuiting Steel
Short Circuiting
Stainless Steel
Aluminum
Argon
X
Argon + 25% CO
2
X
80% or greater Argon +
balance CO
2
or Oxygen
X
X
1
100% CO
2
X
Tri-Mix
2
X
1
Limited short circuiting use
2
90% HE + 7-1/2% AR + 2-1/2% CO
2
Summary of Contents for Handler 210
Page 24: ...OM 227 978 Page 20 6 2 Weld Parameter Chart For 230 VAC Model ...
Page 25: ...OM 227 978 Page 21 227 949 A ...
Page 31: ...OM 227 978 Page 27 Notes ...
Page 32: ...OM 227 978 Page 28 SECTION 8 ELECTRICAL DIAGRAM Figure 8 1 Circuit Diagram ...
Page 33: ...OM 227 978 Page 29 227 951 A ...
Page 43: ...OM 227 978 Page 39 Notes ...
Page 49: ...Notes ...