Tungsten Electrodes

Tungsten is a rare metallic element used for manufacturing TIG welding electrodes. The TIG process relies on tung-

sten’s hardness and high-temperature resistance to carry the welding current to the arc. Tungsten has the highest 

melting point of any metal, 3,410 degrees Celsius.

Tungsten electrodes are nonconsumable and come in a variety of sizes, they are made from pure tungsten or an al-

loy of tungsten and other rare earth elements.  Choosing the correct tungsten depends on the material being welded, 

the amount of amps required and whether you are using AC or DC welding current.

Tungsten electrodes are colour-coded at the end for easy identi cation.

Below are the most commonly used tungsten electrodes found in the New Zealand and Australian market.

Thoriated

Thoriated tungsten electrodes (AWS classi cation EWTh-2) contain a minimum of 97.30 percent tungsten and 1.70 

to 2.20 percent thorium and are called 2 percent thoriated. They are the most commonly used electrodes today and 

are preferred for their longevity and ease of use. Thorium increases the electron emission qualities of the electrode, 

which improves arc starts and allows for a higher current-carrying capacity. This electrode operates far below its melt-

ing temperature, which results in a considerably lower rate of consumption and eliminates arc wandering for greater 

stability. Compared with other electrodes, thoriated electrodes deposit less tungsten into the weld puddle, so they 

cause less weld contamination.

Thorium however is a low-level radioactive hazard and many users have switched to other alternatives. Regard-

ing the radioactivity, thorium is an alpha emitter but when it is enclosed in a tungsten matrix the risks are negligible. 

Thus holding a stick of Thoriated tungsten in your hand should not pose a great threat unless a welder has open cuts 

on their skin. Thoriated tungsten should not get in contact with open cuts or wounds. The more signi cant danger 

to welders can occur when thorium oxide gets into the lungs. This can happen from the exposure to vapours during 

welding or from ingestion of material/dust in the grinding of the tungsten. Follow the manufacturer’s warnings, instruc-

tions, and the Material Safety Data Sheet (MSDS) for its use.

Ceriated (Color Code: Orange)

Ceriated tungsten electrodes (AWS classi cation EWCe-2) contain a minimum of 97.30 percent tungsten and 1.80 to 

2.20 percent cerium and are referred to as 2 percent ceriated. Ceriated tungstens perform best in DC welding at low 

current settings. They have excellent arc starts at low amperages and become popular in such applications as orbital 

tube welding, thin sheet metal work.  They are best used to weld carbon steel, stainless steel, nickel alloys, and 

titanium, and in some cases it can replace 2 percent thoriated electrodes. Ceriated tungsten is best suited for lower 

amperages it should last longer than Thoriated tungsten higher amperage applications are best left to Thoriated or 

Lanthanated tungsten.

Lanthanated (Color Code: Gold)

Lanthanated tungsten electrodes (AWS classi cation EWLa-1.5) contain a minimum of 97.80 percent tungsten and 

1.30 percent to 1.70 percent lanthanum, and are known as 1.5 percent lanthanated. These electrodes have excellent 

arc starting, a low burn off rate, good arc stability, and excellent re-ignition characteristics. Lanthanated tungstens 

also share the conductivity characteristics of 2 percent thoriated tungsten. Lanthanated tungsten electrodes are ideal 

if you want to optimise your welding capabilities. They work well on AC or DC electrode negative with a pointed end, 

or they can be balled for use with AC sine wave power sources. Lanthanated tungsten maintains a sharpened point 

well, which is an advantage for welding steel and stainless steel on DC or AC from square wave power sources.

Zirconiated (Color Code: White)

Zirconiated tungsten electrodes (AWS classi cation EWZr-1) contain a minimum of 99.10 percent tungsten and 0.15 

to 0.40 percent zirconium.  Most commonly used for AC welding Zirconiated tungsten produces a very stable arc and 

is resistant to tungsten spitting. It is ideal for AC welding because it retains a balled tip and has a high resistance to 

contamination. Its current-carrying capacity is equal to or greater than that of thoriated tungsten. Zirconiated tungsten 
is not recommended for DC welding.

Tungsten Electrodes Rating for Welding Currents

 Tungsten 

DC Current Amps 

AC Current Amps 

AC Current Amps

 Diameter 

Torch Negative 

 Un-Balanced Wave 

Balanced Wave

 mm 

2% Thoriated 

0.8% Zirconiated 

0.8% Zirconiated

 1.0mm 

15 - 80 

15 - 80 

20 - 60

 1.6mm 

70 -150 

70 - 150 

60 - 120

 2.4mm 

150- 250 

140 - 235 

100 - 180

 3.2mm 

250 - 400 

225 - 325 

160 - 250

 4.0mm 

400 - 500 

300 - 400 

200 - 320

Содержание KUMJR140DC

Страница 1: ...IG M Lift Arc D Plasma YEARS Warranty Power Source 3 Please read and understand this instruction manual carefully before the installation and operation of this equipment OPERATING MANUAL KUMJR140DC KU...

Страница 2: ...to be invaluable towards the evolution and future development of our equipment range This experience gives us the inside knowledge on what the arc characteris tics performance and interface between ma...

Страница 3: ...rotected from hot metal and sparks Frequently inspect input power cable for wear and tear replace the cable immediately if damaged bare wiring is dangerous and can kill Do not use damaged under sized...

Страница 4: ...plode Because gas cylinders are normally part of the welding process be sure to treat them carefully CYLINDERS can explode if damaged Protect gas cylinders from excessive heat mechanical shocks physic...

Страница 5: ...inside the equipment The machine will be ready for use again when the internal temperature reaches safe level 2 3 Over Voltage Supply Regarding the power supply voltage range of the machine please re...

Страница 6: ...hydrogen The ARC140 is equipped with DC Lift Arc function connection of the 17V Tig torch allows quality DC Tig welding of steel stainless steel bronze and copper The Lift Arc function is superb and...

Страница 7: ...Iron stainless and low hydrogen The ARC170 is equipped with DC Lift Arc function connection of the 17V Tig torch allows quality DC Tig welding of steel stainless steel bronze and copper The Lift Arc f...

Страница 8: ...l MMA TIG Selector Switch Negative Output Terminal Positive Output Terminal Primary Power LED Thermal Alarm LED Primary Input Power Lead On Off Power Switch Rear Machine Layout Description Front Machi...

Страница 9: ...4 Place the electrode into the electrode holder and clamp tight 5 Strike the electrode on the work to create the arc and hold the electrode steady to maintain the arc 6 Hold the electrode slightly abo...

Страница 10: ...across the arc into the molten pool and becomes the deposited weld metal The deposit is covered and protected by a slag which comes from the electrode coating The arc and the immediate area are envelo...

Страница 11: ...ength no greater than the diameter of the core wire Electrode Angle The angle that the electrode makes with the work is important to ensure a smooth even transfer of metal When welding in down hand ll...

Страница 12: ...line of the Tig torch to regulator and connect the regulator to the gas cylinder Carefully open the gas cylinder valve and set the flow rate to between 68 10 l min 5 Set the welding current using the...

Страница 13: ...the work piece 9 With a small movement rotate the Gas Cup forward so that the Tungsten Electrode touches the work piece 10 Now rotate the Gas Cup in the reverse direction to lift the Tungsten electrod...

Страница 14: ...ness and types DC TIG welding is also the cleanest weld with no sparks or spatter LIFT ARC IGNITION for TIG tungsten inert gas Welding Lift Arc is a form of arc ignition where the machines has low vol...

Страница 15: ...pool Travel direction Angle torch Add Tig ller wire Retract the ller wire Move the torch forward to the front of the weld pool Repeat the process gas shield TIG Welding Fusion Technique Manual TIG wel...

Страница 16: ...for its use Ceriated Color Code Orange Ceriated tungsten electrodes AWS classi cation EWCe 2 contain a minimum of 97 30 percent tungsten and 1 80 to 2 20 percent cerium and are referred to as 2 percen...

Страница 17: ...grain running lengthwise and thus grinding crosswise is grinding against the grain If electrodes are ground crosswise the electrons have to jump across the grinding marks and the arc can start before...

Страница 18: ...p long 3a 57Y03 Medium back cap 3b 57Y04 Short back cap 8 HWP17 Torch Handle 150A AIR COOLED TIG WELDING TORCH Rating 150Amp DC 105Amp AC 35 duty cycle For use with non gas solenoid machines 17V TIG T...

Страница 19: ...Alumina Nozzle 19mm 12 Part Description 10N49L Long Alumina Nozzle 8mm 5L 53N48L Long Alumina Nozzle 10mm 6L 53N47L Long Alumina Nozzle 11mm 7L Part Description 54N01 Gas Lens Gasket Part Description...

Страница 20: ...tion Possible Reason Suggested Remedy Insuf cient heat input Increase the amperage or choose a larger electrode Poor welding technique Use the correct welding technique or seek assistance for the corr...

Страница 21: ...e metal Remove materials like paint grease oil and dirt including mill scale from base metal Contaminated ller wire Remove all grease oil or moisture from ller metal Incorrect ller wire Check the ller...

Страница 22: ...nd re grind the tungsten Incorrect tungsten size and or tung sten being used Check and change the size and or the tungsten if required Loose connection Check all connectors and tighten Earth clamp not...

Страница 23: ...6 C09085 Primary Input Cable 17 J09054 Base Plate Part Number Description 1 J10733 Front Plastic Panel 2 J24006 Carry Strap 3 C17001 Tig MMA Selector Switch 4 CX0031 Panel Socket 35 50 5 C14021 Ampera...

Страница 24: ...RANTY RETURNS EXCHANGES 1 Subject to the conditions of warranty set out in warranty period Welding Guns Of Australia PTY LTD warrants that if any defect in any work manship of Welding Guns Of Australi...

Страница 25: ...ng on factors such as the nature of the product and the price Welding Guns Of Australia PTY LTD adopts the same approach As you can appreciate the type of remedy we can offer you may also vary dependi...

Страница 26: ...26...

Страница 27: ...27...

Страница 28: ...112 Christina Rd Villawood NSW 2163 Phone 02 9780 4200 Fax 02 9780 4244 Email sales unimig com au Web www unimig com au Welding Guns Of Australia Pty Ltd ABN 14 001 804 422 UNI FLAME UNI FLAME AUTOLIF...

Отзывы: