11
Examples of comminution tasks
Material
Feeding amount
Material of grinding bowl
and balls
Grinding balls, St. x diam-
eter
Result
Feed size
Grinding bowl size
Grinding duration
Final fineness
Ruby (stone)
140 g
Cr-Ni steel
6 x 30 mm
100%
12 mm
250 ml
3 min
< 250 µm
Titanium dioxide TiO
2
(dry and wet grinding in water)
40 g
Cr-Ni steel
6 x 30 mm
100%
2 mm
250 ml
30 min
< 40 µm
Titanium dioxide TiO
2
(wet grinding in water)
40 g / 50 ml water
Cr-Ni steel
6 x 30 mm
100%
2 mm
250 ml
60 min
< 10 µm
Coal (dry and wet grinding in water)
5 g
Zirconium oxide
5 x 20 mm
100%
0.5 mm
80 ml
120 min
< 15 µm
Aluminium oxide / silicon oxide
100 g
WC + Co
15 x 20 mm
90%
0.1 mm
250 ml
90 min
< 20 µm
Ferrovanadium
70 g
WC + Co
5 x 30 mm
70%
3 mm
250 ml
20 min
< 100 µm
Glass
50 g
Agate
15 x 20 mm
100%
4 mm
250 ml
15 min
< 90 µm
Silicon carbide (dry and wet grinding in water)
15 g
WC + Co
5 x 20 mm
100%
3 mm
80 ml
30 min
< 150 µm
Silicon carbide (dry and wet grinding in water)
15 g / 5 ml water
WC + Co
5 x 20 mm
100%
3 mm
80 ml
45 min
< 71 µm
Examples of comminution tasks
- 60 -
Содержание PULVERISETTE 6 Classic
Страница 55: ...8 2 Device n The planetary mill can be wiped down with a damp cloth when it is switched off Cleaning 55 ...
Страница 65: ...14 Safety logbook Date Maintenance Repair Name Signature Safety logbook 65 ...
Страница 66: ...Date Maintenance Repair Name Signature Safety logbook 66 ...
Страница 69: ......