I
NSTRUCTION
M
ANUAL
3601 E. 34th St. Tucson, AZ 85713 USA Tel. +1 520-882-6598 Fax +1 520-882-6599 email: [email protected] Web: http://www.metallographic.com
42
Please read this instruction manual carefully and follow all installation, operating and safety guidelines.
NANO 1000T / FEMTO 1500
Polishing Head
CLASS 7 Polishing Procedures
5.11.7 Thermal Spray Coatings
The metallographic specimen preparation of thermal spray coatings is
affected by the specimen composition and deposition conditions.
Microstructural features of interest include: porosity, flow, thickness and
inclusions. Proper metallurgical preparation takes into account that the
microstructure may be porous and perhaps somewhat brittle because of
inadequate processing.
Abrasive/surface
Lubricant
FEMTO pressure
setting (psi)
Head / Wheel speed
Time
180 grit SiC paper*
240 grit SiC paper*
Water
5-10 lbs
200/200 rpm
Until plane
1 minute
320 grit SiC paper
400 grit SiC paper
600 grit SiC paper
800 grit SiC paper
1200 grit SiC paper
Water
5 lbs
200/200 rpm
1 minute
1 minute
1 minute
1 minute
3 um DIAMAT diamond on
GOLDPAD polishing pad
DIALUBE
Purple Extender
5 lbs
200/200 rpm
2 minutes
1 um DIAMAT diamond on
ATLANTIS polishing pad
SIAMAT
Colloidal Silica
10 lbs
200/200 rpm
2 minutes
* Recommended for Central Force holders (these steps are not required for Individual Force holders)
Final Polish on Vibratory Polisher using CMP polishing suspension and a MICROPAD polishing pad
Nickel Chrome Coating, Mag 1000x (B.F.)
Nickel-Aluminum Coating, Mag 500x (B.F.)