32
A 22 Order No. BA 93-20-290 Issue 01.03.08
5.7
Checking the Quality of the Weld
You can check the quality of the weld by means of a visual inspection and a bending
test.
See also actual standards in the appendix “Arc stud welding of
metallic materials“, in section irregularities and corrective
actions.
5.7.1
Visual Inspection
A visual inspection must be carried out with each welding element.
Shape, size, evenness, and color of the weld collar are assessed during a visual
inspection. The length of a welded element should be 2 - 3 mm shorter than before
welding.
Condition
Possible cause
Corrective actions
Weld collar evenly, shiny, and complete
Length of w elding element w ithin tolerance
after w elding
- Correct parameters
- None
Contraction of w eld collar
- Plunging depth or lift too low
- Increase plunging depth, check lift and
centering of the ceramic ring
w elding element too long
- Welding energy too high
- Ceramic ring not centered correctly
- Decrease current and/or time
- Check centering
Weakly developed, uneven w eld collar w ith
mat surface
- Welding energy too low
- Increase current and/or time
Welding element too long
- Ceramic ring is humid
- Rebake ceramic rings in a furnace
Single-sided w eld collar
- Arc blow effect
- See arc blow effect
Undercut
- Ceramic ring not centered correctly
- Check centering
Weld collar low , shiny surface w ith many
spatters
- Welding energy too high
- Decrease current and/or time
Welding element too short
- Plunging speed too high
- Adjust plunging depth and/or damping factor
Visual Inspection
Содержание 93-20-290
Страница 1: ...A 22 Welding Gun 93 20 290 Operating Manual...
Страница 45: ...A 22 Order No BA 93 20 290 Issue 01 03 08 45 Welding gun type A 22 ceramic 93 20 290...
Страница 60: ...60 A 22 Order No BA 93 20 290 Issue 01 03 08 Service Support...
Страница 64: ...64 A 22 Order No BA 93 20 290 Issue 01 03 08...
Страница 65: ......