USER MANUAL
SOLDERABILITY TESTER
METRONELEC
V2.0
–
10/2021
6 Avenue Eiffel - 78420 Carrières-sur-Seine
Tél : 01 30 15 20 00
Web :
http://www.metronelec.com| Mail : [email protected]
Page
14
sur
83
The conditions are :
Ageing
: yes
Flux
: type R or RMA Alloy Sn60Pb40 at 245 °C
Immersion speed
20 to 30 mm/s
Immersion depth
4 or 2 mm
Pre heat
: no
Pass / Fail criteria(s)
:
zero crossing time less than 0.59 s (time to across the “x” axis )
Time to obtain 2/3 of the maximum force less than 1.0 s
IEC 68-2-69
This standard defines both methods bath and globule.
Ageing
: defined
Flux
: type R, RMA, RA
Alloy
: Sn60Pb40 at 235 °C or lead free
Immersion speed
: function of the component Immersion depth : function of the
component
Immersion time
: 5 to 10 s.
Pre heat
: no
Pass / Fail criteria(s)
:
Buoyancy crossing time.
Time to obtain 2/3 of the maximum force less than 1.0 s
Minimum of force to reach at 2 and 5 s
IPC/ANSI/J-STD-002/3
This standard defines both methods bath and globule. Solderability test procedures for
components and pcb.
Ageing
: 3 classes defined
Flux
: type R, RMA, RA
Alloy
: Sn60Pb40 at 245 °C or lead free at 255°C Immersion speed : function of the
component
Immersion depth
: function of the component.
Immersion time
: 5 to 10 s.
Immersion angle
: 45 to 70 ° Pre heat : no
Pass / Fail criteria(s)
:
Buoyancy crossing time in less than 1.0 s.
Time to obtain 2/3 of the maximum force less than 1.0 s
Minimum of force to reach at 2 and 5 s
User’s specification
The user can define is own specification pass / fail criteria in time, level of force, time to
buoyancy, etc all criteria defined in standards. See section Utilization.